详细介绍: 钴基焊条
Trade- Mark 牌 号 |
Equivalent to China Standard 相当国标 |
Characteristics & application 特性和用途 |
Equivalent to AWS 相当AWS |
D 802 |
EDCoCr-A-03 |
HRc38-47. Resistance to heat, wear and corrosion. Hardfacing of high temperature part such as the edge of thermo-cutter. HRc38-47,耐热、耐蚀、耐磨。堆焊高温工件如热剪切刀刃 |
ECoCr-A |
D 812 |
EDCoCr-B-03 |
HRc45-50. Resistance to heat, wear and corrosion. Hardfacing of high temperature part such as internal-combustion engine valve. HRc45-50,耐热、耐蚀、耐磨。堆焊高温工件如内燃机阀 |
ECoCr-B |
D 822 |
|
HRc≥53. Resistance to Wear and heat, bad shock resistance. Hardfacing of rotating blade wheel of boiler. HRc≥53,耐热、耐磨,但抗冲击性差。堆焊锅炉旋转叶轮 |
|
D 832 |
EDCoCr-C-03 |
HRc≥50. Wear and heat resistance. Hardfacing of high temperature part such as hot-rolling guided way. HRc≥50,耐热、耐磨。堆焊高温工件如热轧导轨 |
ECoCr-C |
D 842 |
EDCoCr-D-03 |
HRc28-38. Corrosion and thermo-fatigue resistance, work harding. Hardfacing of hot forging die. HRc28-38,耐蚀、抗热疲劳,具有加工硬化性。堆焊热锻模 |
|
D802钴铬钨合金焊芯的钴基堆焊焊条,采用直流反接,堆焊金属在650℃工作仍能保持良好的耐磨性和耐腐蚀性,用于要求在650℃左右工作仍能保持良好的耐磨性和耐腐蚀性的场合,或承受冲击和冷热交错的部位,如堆焊高温高压阀门及热剪切刀刃等。 熔敷金属化学成分/% C-0.70~1.40 Si≤2.0 Mn≤2.0 Cr-25.0~32.0 Fe≤4.0 W-3.0~6.0 其他≤4.0 Co-余量 堆焊层硬度HRC≥40
D812钴基堆焊焊条 D812钴铬钨合金焊芯的钴基堆焊焊条,采用直流反接,堆焊金属在650℃工作仍能保持良好的耐磨性和耐蚀性,用于高温高压阀门、高压泵的轴套筒和内衬套筒以及化钎设备的斩刀刃口等 熔敷金属化学成分/% C-1.00~1.70 Si≤2.00 Mn≤2.00 Cr-25.0~32.0 Fe≤5.0 W-7.0~10.0 其他≤4.0 Co-余量 堆焊层硬度HRC≥44
D822钴基堆焊焊条 D822是高碳钴铬钨合金焊芯的钴基堆焊焊条,采用直流反接,渣覆盖性好,成形美观,具有优良的耐磨、耐热和耐腐蚀性,在650℃高温也能保持这些特性。用于牙轮钻头轴承、锅炉的旋转叶轮、粉碎机刃口.螺旋送料机等磨损部件的堆焊 焊缝金属化学成分(%) C--1.75~3.0 Cr--25.0~33.0 W--11.0~19.0 Mn--≤2.0 Si--≤2.0 Fe--≤5.0 Co--余量 其他总量≤4.0 堆焊层硬度HRC≥53 参考电流: 规格φ(mm) 4.0 5.0 6.0 电流(A) 120~160 140~190 150~210
D842钴基堆焊焊条 说明:钴基4号低碳钴铬钨合金焊芯的堆焊焊条,采用直流反接,堆焊金属在800℃仍能保持良好的看热疲劳性和耐蚀性。 用途:用于高温条件下承受冲击和冷热交错的工件堆焊,如热锻模,阀门密封面等,具有良好的性能。 熔敷金属化学成分/% C Si Mn Cr Fe W 其他 Co 0.20~0.50 ≤2.00 ≤2.00 23.0~32.0 ≤5.00 ≤9.50 ≤7.00 余量
|